Grado de General
Transparentes,
No sellable de calor
Propiedades | MéTodo de ensayo | Unidad | El valor tíPico | |||||
Grosor | Kincess | ΜM | 18 | 20 | 30 | 40 | 60 | |
VariacióN del espesor | La norma ASTM-252-78 | % | ±3.0 | ±3.0 | ±2,5 | ±2.0 | De ±1,5 | |
El rendimiento | Kincess | M 2 /kg. | 61.1 | 55,0 | 36.6 | 27.5 | 18.4 | |
Fuerza tensil | MD | La norma ASTM D-882 | MPa | 150 | 150 | 160 | 145 | 140 |
TD | La norma ASTM D-882 | MPa | 300 | 300 | 300 | 280 | 280 | |
La elongacióN en el recreo | MD | La norma ASTM D-882 | % | 170 | 170 | 170 | 175 | 180 |
TD | La norma ASTM D-882 | % | 50 | 50 | 55 | 55 | 60 | |
Coeficiente de friccióN | T/T-EE.UU. | La norma ASTM D-1894 | 0.35 | 0.35 | 0.35 | 0.35 | 0.35 | |
T/S O EE.UU. | La norma ASTM D-1894 | 0.40 | 0.40 | 0.40 | 0.40 | 0.40 | ||
El Encogimiento de calor | MD | La norma ASTM D-1204 | % | 4.0 | 4.0 | 4.0 | 4.0 | 4.0 |
TD | La norma ASTM D-1204 | % | 2.0 | 2.0 | 2.0 | 2.0 | 2.0 | |
Haze | La norma ASTM D-1003 | % | 1.0 | 1.0 | 1.1. | 1.2 | 1.5 | |
Gloss | La norma ASTM D-2457 | 90 | 90 | 90 | 90 | 90 | ||
Mojar la tensióN | La norma ASTM D-2578 | Dyn | 38 | 38 | 38 | 38 | 38 |